On the production floor of rubber compression molding, the most nerve-wracking sound is often the faint "hiss" at the moment the mold opens—it usually means a perfectly good part has been torn at the parting line or in a dead corner, or even had a chunk ripped off. Demolding tears not only directly drive up scrap rates but also severely disrupt the rhythm of continuous production.
When many front-line engineers face this problem, their first instinct is often to blame "improper mold release agent application," but the reality is far more complex. Demolding tears are fundamentally a systemic problem involving the physical properties of the compound at high temperature, the geometric design of the mold, precise control of the cure state, and interfacial tribology. Below, we break down the major core causes of rubber demolding tears one by one in a Q&A format and provide targeted troubleshooting approaches.
A: This is a typical combined effect of insufficient "hot tear strength" and loss of mold temperature control.
When formulation engineers measure tear strength in the lab, the data often looks great—but that is data at room temperature (23°C). At the moment of demolding, rubber products are at 150°C–180°C, where intensified thermal motion of the rubber molecular chains puts physical properties in their most vulnerable window. Experienced data show that the tear strength of rubber at 150°C may be only one-third or even lower than at room temperature.
If the formulation uses large amounts of reclaimed rubber for cost reduction, or has excessive oil loading, the compound's "skeleton" strength at high temperature is extremely poor and tears at the slightest pull. In addition, if the mold temperature controller fails or continuous production overheats the mold (e.g., above 185°C), the compound not only becomes more prone to sticking but its high-temperature embrittlement tendency also increases sharply—forcing demolding at this point makes tearing almost inevitable. The countermeasure is to verify the compound's high-temperature tear performance and strictly keep the mold working temperature within the process window (e.g., 165°C–175°C); before demolding, cold air can be used to cool the part slightly to increase compound rigidity.
A: The problem often lies in "geometric stress concentration," not surface finish.
The physical essence of demolding tears is: the local stress generated at the moment of demolding exceeds the tear strength of the compound at that temperature. When the mold has sharp R corners, deep undercuts, or extremely thin wall transition zones, the rubber must undergo severe elastic deformation to "squeeze" out during ejection or mold opening. If the R corner is too small, stress becomes highly concentrated at a single point, and the tear starts there.
Insufficient draft angle is also a hidden killer. If the sidewall is vertical or the draft is less than 1°, the friction resistance between rubber and mold wall surges, and forced ejection inevitably tears thin walls or boss areas. The recommendation is to enlarge R corners as much as possible without affecting product function and to ensure sufficient draft angle; for deep undercut structures that are extremely prone to tearing, it may be necessary to evaluate whether a tear-trim mold design or an auxiliary demolding mechanism should be added.
A: What you see as "sufficient time" may be an illusion—the actual state of cure may not meet spec.
Undercure is one of the most insidious culprits behind demolding tears. When the crosslink network inside the compound is not yet fully formed, the rubber is like ice that hasn't frozen solid—macroscopically it appears formed, but microscopically its strength is extremely low. There are many causes of undercure: beyond the obvious short cure time, a compound scorch time that is too short causes loss of flow (it sets before filling the cavity), poor venting leads to local short shots, or uneven dispersion of ingredients (e.g., sulfur) all result in locally insufficient cure.
During front-line troubleshooting, don't just look at the time setting. It is advisable to spot-check the state of cure with an RPA (Rubber Processing Analyzer); if the cure state is below 90%, the crosslink density is insufficient, and forced demolding will inevitably cause tears. At the same time, check whether the compound has a scorch tendency—scorched compound cannot flow inside the mold, resulting in poor compactness, delamination, and shrinkage of the product.
A: Mold release agent is not "the more the better"—wrong selection or over-spraying can backfire.
The role of the release agent is to form a low-surface-energy release film between the mold and the rubber. However, if sprayed too thickly or over-applied in localized areas, this film may migrate or accumulate under clamping pressure and high temperature, causing oily blotches on the product surface and even affecting subsequent painting or bonding. More critically, selection mismatch: for example, when producing silicone rubber products, if an ordinary silicone-oil-based release agent is mistakenly used, the "like dissolves like" principle causes the release agent to penetrate into the silicone rubber instead, worsening mold sticking—the more you spray, the more it sticks.
The correct approach: select a release agent matched to the rubber type (e.g., water-based semi-permanent for EPDM/NR; high-temperature fluorine-containing types for FKM), keep a spray distance of 15–20 cm, aim for "moist but not wet," and ensure the solvent fully evaporates and dries before closing the mold. If the mold surface already has stubborn silicone oil carbon buildup or scale, simply spraying more release agent is ineffective—the mold must first be thoroughly cleaned or sandblasted.
A: Rough mold-opening technique and improper compound placement are the last straw that breaks the product.
In many small and medium-sized factories, peaks in demolding tears often coincide with shift changes or new operators. If an operator pries from only one side with uneven force during mold opening, or blasts an air gun directly at a weak spot, the instantaneous mechanical impact far exceeds the compound's limit, and tearing is unavoidable. In addition, incorrect compound placement or insufficient compound weight causes local short shots in the cavity; that area receives insufficient curing pressure during clamping, has inherently lower strength, and naturally tears from the short-shot area during demolding.
The management-level countermeasures are simple but often overlooked: establish a standard demolding work instruction and train operators to open molds with even, gentle force; use brass or plastic pry bars dedicated to complex molds; and strictly spot-check and weigh compound charges to ensure proper flash allowance (typically 15%–20% overfill for compression molds to drive out air and maintain pressure).
Summary
Rubber demolding tears are never a "terminal illness" caused by a single factor. When facing a batch of torn scrap, try troubleshooting in this order: first check mold temperature and state of cure (process) → then examine R corners and undercuts (mold) → verify hot tear strength (formulation) → finally review release agent and operating technique (shop floor). Only by reducing the instantaneous stress at the moment of demolding, or increasing the compound's tear strength at high temperature, can you fundamentally protect the yield rate at that "final kick."
[RUBBER MOLD] In-Depth Analysis: The Major Causes of Tearing Dur......
2026-11-09
[RUBBER] How to Reduce the Shrinkage Rate of TPV Rubber
2026-10-12
[RUBBER] Rubber Technology Basic Knowledge: From Molecular ......
2026-09-07
[RUBBER] Classification of Rubber: From Natural Rubber to S......
2026-08-24